The common injection moulding defects are sink marks, warpage, short shots, flash, weld lines, burn marks, voids and splay. Most come from uneven wall thickness, trapped air, poor cooling or the wrong process settings, so a design review before the mould is cut prevents many of them.

Eight common defects appear in injection moulding: sink marks, voids, warpage, short shots, flash, weld lines, burn marks and splay. They sit among 24 injection moulding problems in engineering thermoplastics, and most stem from uneven wall thickness, poor cooling, trapped gas, wet resin or machine settings. Knowing what causes each fault tells you whether a press adjustment will resolve it or whether the part design or mould needs changing.

DefectWhat you seeMain causeMain fix
Sink marksDip opposite ribs, bosses or thick wallsUneven walls, differing shrinkage, low packing, hot spots, fast fillUniform walls, thinner rib bases, better cooling and packing
VoidsHollow pockets inside thick wallsThick walls, non-uniform cooling, low packing, hot spots, fast fillReduce thick sections, improve cooling and packing
WarpagePart distorts after ejection or laterDiffering shrinkage, uneven cooling, fibre orientation, residual stressUniform walls and balanced mould cooling
Short shotsIncomplete partResin does not fill the mould completelyAdjust process settings or review part and mould design
FlashExcess plastic escaping the cavityInadequate clamp tonnage, core shift, high fill speed or pressure, low melt temperatureWell-fitted mould, adequate clamp force, corrected settings
Weld linesVisible line where melt fronts meetMelt fronts meeting inside the cavityMove gates, tune settings or run a mould flow study
Burn marksBurnt resin where gas is trappedTrapped air and volatile gas compressed until it burns resinAdd venting, clean clogged vents, lower injection speed
SplaySurface streaks from steam bubblesExcess residual moisture in the granulesDry the material below its moisture limit

What causes sink marks and voids in injection moulded parts?

Sink marks and voids both come from uneven or overly thick walls, poor cooling and packing faults during moulding. Where wall thickness differs, sink marks appear on the visible face opposite ribs and bosses due to differing shrinkage during cooling. Voids form inside thick walls too.

Process settings contribute too, as insufficient packing, mould hot spots and injection that is too fast drive both sinks and voids. Keeping walls uniform avoids thick junctions that press settings cannot fix later. Size each rib base to about half the wall thickness with rib height limited to 3 times the wall thickness, and check how thin injection moulded parts can be early in CAD.

What causes warpage in injection moulded parts?

Warpage occurs when sections of a moulded part shrink unevenly and pull the part out of shape. Shrinkage differences between thin and thick sections, uneven cooling, fibre orientation and residual stress all cause distortion, which can appear long after moulding.

Moulded-in residual stresses can warp a part after ejection, and fibre orientation adds directional shrinkage in glass-filled resins. Cooling layout directly affects flatness as well, since poor mould cooling increases cycle time, uneven cooling, residual stress and warpage. Uniform walls and balanced cooling channels address distortion at its source.

What causes flash and short shots in injection moulding?

Flash comes from inadequate clamp tonnage, core shift, fill speed or pressure that is too high, or melt temperature that is too low, while a short shot happens when molten resin does not fill the mould completely. Stopping flash requires a well-fitted mould alongside adequate clamp force and corrected fill and temperature settings.

Short shots leave incomplete parts where melt stops short inside the cavity. Related surface issues such as flow marks come from low mould or resin temperature or insufficient holding pressure. Process adjustments often resolve fill faults, though poor mould fit or restrictive part geometry still calls for tooling or design changes.

What causes weld lines, burn marks and splay in injection moulded parts?

Weld lines come from meeting melt fronts, burn marks from trapped gas and splay from wet resin. Where separate melt fronts merge, weld lines and air traps form; because a weld line is often unavoidable, engineers tune process settings to soften its look or adjust gate positions to move it onto a less visible face.

Burn marks occur when trapped air and volatile gas compress in the cavity until they burn the resin. When air cannot escape through parting lines, ejectors or venting inserts, adequate venting, cleaning clogged venting channels and lowering injection speed prevent scorching. Splay leaves surface streaks when excess residual moisture in the granules creates steam bubbles, resolved by drying the resin below its moisture limit.

How does design for injection moulding prevent defects before the mould is cut?

Reviewing part geometry before cutting steel prevents structural faults that press settings cannot fix later. A mould flow study before the mould is built flags where melt fronts meet so gate placement and venting can be set early, and a design for manufacturing review checks wall uniformity, rib ratios and cooling layout.

Fixing thick sections and cooling before machining avoids reworking steel.

How does Lianto Plastics check for injection moulding defects?

Lianto reviews the design for these faults before tooling, and first samples come with a measurement report and photos so you can check the part. A 3D printed prototype can prove the shape first. Send your files through the quote form.

Questions

What is the most common injection moulding defect?

Sink marks, warpage and short shots are among the most commonly discussed. Sink marks and warpage mostly trace back to uneven wall thickness and cooling.

Can injection moulding defects be fixed after the mould is cut?

Some process-related defects can be corrected by changing settings. Others, such as sink marks from thick sections, usually need a design or mould change, which is why a design review before tooling matters.

What causes warpage in plastic parts?

Warpage comes from differing shrinkage between thin and thick sections, uneven cooling, fibre orientation and residual stress in the part.

How do you stop flash on an injection moulded part?

Flash is linked to inadequate clamp force, core shift, too high a fill speed or pressure, and too low a melt temperature. A well-fitted mould and correct settings address it.

Sources

  1. Predicting molding defects using injection molding analysis, Asahi Kasei Engineering Plastics

  2. Injection-Molding Problems in Engineering Thermoplastics: Causes and Solutions, BASF

  3. Injection molding troubleshooting guide for Eastman copolyesters, Eastman

  4. Part and mold design guide for Eastman polymers, Eastman

  5. Wall thickness in injection moulded parts, Envalior

Got an idea or a drawing?